Technology · Durability Data
Durability and Process Window Data
An interior adhesive has two jobs: survive ten years of heat, humidity and sunlight in the cabin, and run cleanly on your line every shift. This page collects RELANET's test data for both: yellowing, heat and humidity aging, thermal cycling, initial tack, open time and activation window. Each value comes with the product, the test condition and the source.
It covers RELANET's non-yellowing and hydrolysis-resistant interior adhesives.

ΔE ≈ 1.0
RY-10 color change after 110°C × 1,500 h
85%
R-5670 peel retention after 60°C / 95% RH × 1,000 h
91.3%
PUR peel retention after 85°C / 95% RH × 1,000 h
110–140°C
Activation window, R-5670 automated-line version
The Problem
Most Interior Bonds Don't Fail on Day One
They fail after the first summer, or on the line when the oven drifts. The failure modes are well known:
Yellowing. Light-colored skins and backlit trim turn yellow when the adhesive layer isn't light-stable.
Hydrolysis. In hot, humid climates, moisture slowly breaks down the bond line. The film turns white, swells and lets go.
Heat creep and blistering. A closed car in summer gets hot enough to soften the adhesive. Edges lift and skins bubble.
Cold cracking. In winter workshops and cold climates the adhesive film loses elongation and cracks at radii.
A narrow process window. Small swings in oven temperature, open time or lamination timing turn into a batch of rejects.
The data below shows how each RELANET adhesive handles these risks.
Anti-Yellowing
Non-Yellowing Adhesives for White Interiors and Backlit Trim
Why some adhesives yellow. Polyurethanes made from aromatic isocyanates contain benzene rings that oxidize under heat and UV light, so the film darkens over time. RELANET's light-transmitting and interior PU adhesives use aliphatic chemistry, which has no aromatic ring to oxidize. That matters most on white, beige and light-gray skins and on any part with light shining through it.
Below is the data for each RELANET non-yellowing adhesive for automotive interior parts: product, test condition, result and source.
| Product | Test | Result | Source |
|---|---|---|---|
| RY-10 optical hot-melt film | 110°C × 1,500 h | ΔE ≈ 1.0 | Formal project test report; in series production on Honda Ye P7 / Ye S7 |
| R-60 optical film | QUV, 1,500 h | ΔYi ≤ 1 | Typical lab value |
| R-5610 optical waterborne PUD | 85°C heat aging, 1,600 h | ΔYI −0.17 (table below) | Typical lab value |
| R-5670 2K waterborne PU | 85°C × 500 h + UV 300 h | ΔE < 1.2, no visible yellowing | Typical lab value |
| R-5610 high-transmittance anti-yellowing waterborne PUD | 120°C; 85°C / 85% RH; 1,000 h | Passed | GAC R&D Center testing, March 2026 |
- Test
- 110°C × 1,500 h
- Result
- ΔE ≈ 1.0
- Source
- Formal project test report; in series production on Honda Ye P7 / Ye S7
- Test
- QUV, 1,500 h
- Result
- ΔYi ≤ 1
- Source
- Typical lab value
- Test
- 85°C heat aging, 1,600 h
- Result
- ΔYI −0.17 (table below)
- Source
- Typical lab value
- Test
- 85°C × 500 h + UV 300 h
- Result
- ΔE < 1.2, no visible yellowing
- Source
- Typical lab value
R-5610 high-transmittance anti-yellowing waterborne PUD
- Test
- 120°C; 85°C / 85% RH; 1,000 h
- Result
- Passed
- Source
- GAC R&D Center testing, March 2026
R-5610 yellowness over 1,600 hours at 85°C
| Aging time | L | a | b | ΔYI |
|---|---|---|---|---|
| Reference | 99.95 | 0.03 | −0.01 | 0.01 |
| 500 h | 104.36 | 0.01 | −0.13 | −0.22 |
| 750 h | 104.72 | −0.01 | −0.18 | −0.31 |
| 1,000 h | 104.51 | 0.00 | −0.17 | −0.29 |
| 1,600 h | 104.17 | −0.03 | −0.09 | −0.17 |
Reference
- L
- 99.95
- a
- 0.03
- b
- −0.01
- ΔYI
- 0.01
500 h
- L
- 104.36
- a
- 0.01
- b
- −0.13
- ΔYI
- −0.22
750 h
- L
- 104.72
- a
- −0.01
- b
- −0.18
- ΔYI
- −0.31
1,000 h
- L
- 104.51
- a
- 0.00
- b
- −0.17
- ΔYI
- −0.29
1,600 h
- L
- 104.17
- a
- −0.03
- b
- −0.09
- ΔYI
- −0.17
ΔYI stays within ±0.31 across 1,600 hours, and the b value (yellow–blue axis) never turns positive.

- Reference0.01
- 500 h−0.22
- 750 h−0.31
- 1,000 h−0.29
- 1,600 h−0.17
Designing backlit trim? See illuminated interior trim solutions
Heat and Humidity Resistance
Hydrolysis-Resistant Automotive Adhesives
Why some adhesives hydrolyze. Ester bonds in conventional polyester polyurethanes react with water over time, especially when hot. R-5670 uses a polycarbonate-modified backbone, which is far harder for water to break. RELANET PUR builds a dense crosslinked network for the same reason. The result is a bond line that stays clear and strong after long humidity aging.
Waterborne PU (R-5670)
| Test | Result | Source |
|---|---|---|
| 60°C / 95% RH × 1,000 h | 85% peel retention; film clear, no whitening or swelling | Typical lab value |
| −40°C × 24 h | 92% peel retention | Typical lab value |
| 105°C × 24 h | 88% peel retention | Typical lab value |
| 85°C × 500 h | No color change, no bleeding or migration into the skin | Typical lab value |
| 72 h immersion in neutral interior cleaner and silicone care fluid | <6% strength loss; no swelling | Typical lab value |
| Vacuum forming at −0.09 to −0.1 MPa | No slipping or delamination of the film under sustained stretch | Typical lab value |
60°C / 95% RH × 1,000 h
- Result
- 85% peel retention; film clear, no whitening or swelling
- Source
- Typical lab value
−40°C × 24 h
- Result
- 92% peel retention
- Source
- Typical lab value
105°C × 24 h
- Result
- 88% peel retention
- Source
- Typical lab value
85°C × 500 h
- Result
- No color change, no bleeding or migration into the skin
- Source
- Typical lab value
72 h immersion in neutral interior cleaner and silicone care fluid
- Result
- <6% strength loss; no swelling
- Source
- Typical lab value
Vacuum forming at −0.09 to −0.1 MPa
- Result
- No slipping or delamination of the film under sustained stretch
- Source
- Typical lab value
OEM interior test: BYD HTE spare-wheel cover (R-5670 + R-60C)
| Test | Condition | Average peel | Failure mode | Judgment |
|---|---|---|---|---|
| Room temperature | 23 ± 3°C, 55% RH | 28.8 N | Substrate failure (all 3) | Pass |
| Heat aging | 90 ± 2°C × 168 h, then 1 h at RT | 30.7 N | Substrate failure (all 3) | Pass |
| Cyclic damp heat | (80°C × 15.5 h → RT 0.5 h → −40°C × 7.5 h → RT 0.5 h) × 10 cycles, then 1 h at RT | 29.5 N | Substrate failure (all 3) | Pass |
Room temperature
- Condition
- 23 ± 3°C, 55% RH
- Average peel
- 28.8 N
- Failure mode
- Substrate failure (all 3)
- Judgment
- Pass
Heat aging
- Condition
- 90 ± 2°C × 168 h, then 1 h at RT
- Average peel
- 30.7 N
- Failure mode
- Substrate failure (all 3)
- Judgment
- Pass
Cyclic damp heat
- Condition
- (80°C × 15.5 h → RT 0.5 h → −40°C × 7.5 h → RT 0.5 h) × 10 cycles, then 1 h at RT
- Average peel
- 29.5 N
- Failure mode
- Substrate failure (all 3)
- Judgment
- Pass
Specimens: flocked fabric on sand-blasted PHC paper honeycomb. 80 g/m² per side, dried 80°C × 5 min, pressed 0.2 MPa × 15 s, cured 7 days. Report RJTSC-26-7-2-001, tested against the BYD interior standard. Peel strength did not drop after aging; every specimen broke in the material, not the bond.
Reactive PUR hot melt (R-series)
| Test | Result | Source |
|---|---|---|
| 85°C / 95% RH × 1,000 h | ≥91.3% strength retention (8.7% loss) | Third-party tested; report on request |
| 105°C × 168 h | ≥92% strength retention | Third-party tested; report on request |
| Service temperature range | −40°C to 110°C | Third-party tested; report on request |
85°C / 95% RH × 1,000 h
- Result
- ≥91.3% strength retention (8.7% loss)
- Source
- Third-party tested; report on request
105°C × 168 h
- Result
- ≥92% strength retention
- Source
- Third-party tested; report on request
Service temperature range
- Result
- −40°C to 110°C
- Source
- Third-party tested; report on request
- R-5670 (60°C / 95% RH)85%
- R-series PUR (85°C / 95% RH)91.3%
RELANET data only; each bar is labeled with its own test condition.
Other grades
| Product | Heat resistance | Source |
|---|---|---|
| R-5610 | 110°C × 168 h | Product data |
| R-7206 APAO | Stable long term at 110°C; no debonding at 110°C in a specific project | Product data; project report RCTSC-25-10-18-001 |
| R-7110 APAO | Designed for 90°C; for areas without direct sunlight | Product data |
| R-5110 waterborne chloroprene | See TDS | — |
- Heat resistance
- 110°C × 168 h
- Source
- Product data
- Heat resistance
- Stable long term at 110°C; no debonding at 110°C in a specific project
- Source
- Product data; project report RCTSC-25-10-18-001
- Heat resistance
- Designed for 90°C; for areas without direct sunlight
- Source
- Product data
- Heat resistance
- See TDS
- Source
- —
Thermal Cycling
From Winter Cold to Summer Heat
| Product | Cycle | Result | Source |
|---|---|---|---|
| R-5670 | −40°C ↔ 105°C, 100 cycles | No delamination; 85% peel retention | Typical lab value |
| Waterborne PUD (automotive grades) | −40°C × 4 h → 90°C × 4 h, 50 cycles | ≥88% peel retention; no whitening, embrittlement, shrinkage or debonding | Typical lab value |
| R-series PUR | −40°C ⇌ 90°C, 500 cycles | Bond line intact, no debonding | Third-party tested; report on request |
| RY-10 | −40°C to 110°C cycling + UV aging | Transmittance and adhesion retained | Product data |
- Cycle
- −40°C ↔ 105°C, 100 cycles
- Result
- No delamination; 85% peel retention
- Source
- Typical lab value
Waterborne PUD (automotive grades)
- Cycle
- −40°C × 4 h → 90°C × 4 h, 50 cycles
- Result
- ≥88% peel retention; no whitening, embrittlement, shrinkage or debonding
- Source
- Typical lab value
R-series PUR
- Cycle
- −40°C ⇌ 90°C, 500 cycles
- Result
- Bond line intact, no debonding
- Source
- Third-party tested; report on request
- Cycle
- −40°C to 110°C cycling + UV aging
- Result
- Transmittance and adhesion retained
- Source
- Product data
Cold-workshop elongation. At 10°C, the hand-wrapping version of R-5670 keeps 600–1,000% elongation at break (ASTM D412, typical lab value), so skins stretched over armrest radii don't tear the film. R-series PUR reaches ≥500%.
Process Window
Long Open Time, Wide Activation Window, Fast Initial Tack
A wide process window means the adhesive tolerates normal swings in oven temperature, operator speed and line timing without producing rejects.
Both versions of R-5670 are long open time waterborne adhesives, and the automated-line version is a wide activation window adhesive (110–140°C).
R-5670 2K waterborne PU: two versions for two processes
| Parameter | Hand-wrapping version | Automated-line version |
|---|---|---|
| Open time | 8–15 min | 5–10 min |
| Activation | 65–85°C (low-temperature activation protects thin leather and light skins) | Wide window 110–140°C; full green strength in 40–60 s at 120–130°C |
| Drying | Surface dry 10–25 min at room temperature, or 3–8 min in an 80°C oven | Staged oven drying, 60°C → 80°C, to avoid skin shrinkage |
| Coat weight | 80–110 g/m² per side | See TDS |
| Mix ratio | R-5670 : R-60C = 100 : 5–8 (by weight) | Same |
| Initial tack | About 25 N/25 mm at 1 minute after lamination | Same |
| Next step | Full crosslinking after 24 h at 23°C | Parts can go to assembly after 12 h of natural curing |
| Vacuum hold | — | 40–90 s, so the film stretches with the skin and air escapes from 3D curves |
Open time
- Hand-wrapping version
- 8–15 min
- Automated-line version
- 5–10 min
Activation
- Hand-wrapping version
- 65–85°C (low-temperature activation protects thin leather and light skins)
- Automated-line version
- Wide window 110–140°C; full green strength in 40–60 s at 120–130°C
Drying
- Hand-wrapping version
- Surface dry 10–25 min at room temperature, or 3–8 min in an 80°C oven
- Automated-line version
- Staged oven drying, 60°C → 80°C, to avoid skin shrinkage
Coat weight
- Hand-wrapping version
- 80–110 g/m² per side
- Automated-line version
- See TDS
Mix ratio
- Hand-wrapping version
- R-5670 : R-60C = 100 : 5–8 (by weight)
- Automated-line version
- Same
Initial tack
- Hand-wrapping version
- About 25 N/25 mm at 1 minute after lamination
- Automated-line version
- Same
Next step
- Hand-wrapping version
- Full crosslinking after 24 h at 23°C
- Automated-line version
- Parts can go to assembly after 12 h of natural curing
Vacuum hold
- Hand-wrapping version
- —
- Automated-line version
- 40–90 s, so the film stretches with the skin and air escapes from 3D curves
Typical lab values. Initial tack measured on PVC with knitted backing laminated to flame-treated PP, 25 mm width, timed from the end of lamination; about 60 N/25 mm after 7 days.
Why each parameter matters on the line
- Long open time (8–15 min): operators have time to reposition the skin around curved armrests and deep corners without trapping air or creasing the skin.
- Wide activation window (110–140°C): a 30°C window means oven drift on an automated line doesn't change green strength, so the first and last part of a shift bond the same way.
- Fast initial tack (25 N/25 mm at 1 minute): parts can be demolded and handled sooner, which shortens the cycle and stops skins from springing back at edges.
Activation temperature (°C)
- Hand-wrapping version: 65–85°C, 8–15 min
- Automated-line version: 110–140°C, 5–10 min
Redrawn from the data on this page.

Other grades
| Product | Open time | Activation / application | Initial strength | Source |
|---|---|---|---|---|
| R-5610 optical waterborne PUD | See TDS | Activation above 60°C; drying 50–70°C × 8–15 min | See TDS | R-5610 TDS ver. 25.6 |
| R-5110 waterborne chloroprene | Bond immediately after spraying | Press 1–10 s at 20°C | Fast tack on porous materials | R-5110 TDS ver. 25.6 |
| R-7110 APAO | 1–2 min at 180°C (long, for positioning large parts) | Applied at 180°C | See TDS | APAO TDS |
| R-7206 APAO | About 1–2 min at 180°C | Applied at 180°C; fast strength build-up for robotic lines | See TDS | TDS |
| R-9610 PUR | 45–90 s at 23°C | Melt viscosity 6,200–9,000 mPa·s at 120°C | 28–36 N/25 mm initial 180° peel | Third-party tested; report on request |
| RY-10 optical film | Preformed film, activated at the press | Infrared activation, then 35 s pressing; no vacuum de-bubbling | About 45 N/25 mm at 1 minute | Product data |
- Open time
- Bond immediately after spraying
- Activation / application
- Press 1–10 s at 20°C
- Initial strength
- Fast tack on porous materials
- Source
- R-5110 TDS ver. 25.6
- Open time
- 1–2 min at 180°C (long, for positioning large parts)
- Activation / application
- Applied at 180°C
- Initial strength
- See TDS
- Source
- APAO TDS
- Open time
- About 1–2 min at 180°C
- Activation / application
- Applied at 180°C; fast strength build-up for robotic lines
- Initial strength
- See TDS
- Source
- TDS
- Open time
- 45–90 s at 23°C
- Activation / application
- Melt viscosity 6,200–9,000 mPa·s at 120°C
- Initial strength
- 28–36 N/25 mm initial 180° peel
- Source
- Third-party tested; report on request
- Open time
- Preformed film, activated at the press
- Activation / application
- Infrared activation, then 35 s pressing; no vacuum de-bubbling
- Initial strength
- About 45 N/25 mm at 1 minute
- Source
- Product data

One window that isn't on the adhesive datasheet. After flame or plasma treatment, PP must be laminated within about 4 hours. After that, active groups on the surface fade even though the dyne reading still looks fine. We write this time window into the process instruction, next to the oven settings.
Curing Stages
From Lamination to Full Strength
| Stage | What it means | R-5670 (2K waterborne PU) | R-9610 (reactive PUR) | RY-10 (film) |
|---|---|---|---|---|
| Open time | Time to place and adjust the skin after coating or activation | 8–15 min (hand) / 5–10 min (automated) | 45–90 s | Activated by IR at the press |
| Initial tack (green strength) | Strength right after lamination, so the part can be handled | ~25 N/25 mm at 1 min | Physical set on cooling; 28–36 N/25 mm | ~45 N/25 mm at 1 min |
| Handling / next process | Part can move to the next station | After 12 h natural curing (automated version) | See TDS | After pressing and cooling |
| Full cure | Final strength and heat resistance | Full crosslinking 24 h at 23°C; ~60 N/25 mm at 7 days | Moisture cure, 7 days | See TDS |
Open time
- What it means
- Time to place and adjust the skin after coating or activation
- R-5670 (2K waterborne PU)
- 8–15 min (hand) / 5–10 min (automated)
- R-9610 (reactive PUR)
- 45–90 s
- RY-10 (film)
- Activated by IR at the press
Initial tack (green strength)
- What it means
- Strength right after lamination, so the part can be handled
- R-5670 (2K waterborne PU)
- ~25 N/25 mm at 1 min
- R-9610 (reactive PUR)
- Physical set on cooling; 28–36 N/25 mm
- RY-10 (film)
- ~45 N/25 mm at 1 min
Handling / next process
- What it means
- Part can move to the next station
- R-5670 (2K waterborne PU)
- After 12 h natural curing (automated version)
- R-9610 (reactive PUR)
- See TDS
- RY-10 (film)
- After pressing and cooling
Full cure
- What it means
- Final strength and heat resistance
- R-5670 (2K waterborne PU)
- Full crosslinking 24 h at 23°C; ~60 N/25 mm at 7 days
- R-9610 (reactive PUR)
- Moisture cure, 7 days
- RY-10 (film)
- See TDS
R-5670 (2K waterborne PU)
- 1Open time8–15 min (hand) / 5–10 min (automated)
- 2Initial tack (green strength)~25 N/25 mm at 1 min
- 3Handling / next processAfter 12 h natural curing (automated version)
- 4Full cureFull crosslinking 24 h at 23°C; ~60 N/25 mm at 7 days
R-9610 (reactive PUR)
- 1Open time45–90 s
- 2Initial tack (green strength)Physical set on cooling; 28–36 N/25 mm
- 3Handling / next processSee TDS
- 4Full cureMoisture cure, 7 days
RY-10 (film)
- 1Open timeActivated by IR at the press
- 2Initial tack (green strength)~45 N/25 mm at 1 min
- 3Handling / next processAfter pressing and cooling
- 4Full cureSee TDS
Built for Hot, Humid Climates
Tested Where Humidity Is the Daily Condition
RELANET is based in Guangzhou, where summers are hot and humid for months at a time. Our humidity-aging tests (60°C / 95% RH and 85°C / 95% RH, 1,000 h) and cyclic damp-heat tests reflect that climate. Conditions in much of Brazil and Southeast Asia are similar, so the same data applies when you build or ship interior parts there.
Humid workshops also affect the process: waterborne adhesives dry more slowly and parts can blush (turn white) after lamination. Our engineers adjust solids, activation temperature and open time to your plant's climate and equipment, on site if needed.
How to Use This Data
Read Accelerated Aging Results Correctly
- Accelerated aging is a comparison tool, not a lifetime prediction. 1,000 hours in a humidity chamber can't be converted into years in a car. Use the results to compare adhesives under the same condition, and validate the finished part to your OEM's standard.
- Results depend on the material pair. The same adhesive gives different peel values on different skins and substrates. Typical lab values apply to the specimens described.
- Compare like with like. A retention figure after 60°C / 95% RH isn't comparable with one after 85°C / 95% RH, and a ΔE value isn't the same as ΔYI.
- Lab data is not a production guarantee. Before SOP, we run the tests on your parts, your materials and your line settings.
We Tune the Window to Your Line
Custom Open Time, Activation Temperature and Tack
If a standard grade doesn't fit your oven, cycle time or climate, we adjust the formula: open time, activation temperature, solids and the balance between initial tack and final strength. Custom samples for difficult substrates are ready in 7 working days.
- 01
You send the process data: equipment, oven settings, cycle time, skin and substrate.
- 02
We test flat panels and recommend a grade or a custom version.
- 03
We trial it on your line and record coat weight, temperature and timing.
- 04
We hand over a process instruction with the validated window.
Frequently Asked Questions
Which RELANET adhesives are non-yellowing?
RY-10 film (ΔE ≈ 1.0 after 110°C × 1,500 h), R-60 film (ΔYi ≤ 1 after 1,500 h QUV), R-5610 waterborne PUD (ΔYI −0.17 after 1,600 h at 85°C) and R-5670 (ΔE < 1.2 after 85°C × 500 h + UV 300 h). All use aliphatic chemistry.
Is R-5670 hydrolysis resistant?
Yes. It keeps 85% of its peel strength after 1,000 h at 60°C / 95% RH, with no whitening or swelling, thanks to a polycarbonate-modified backbone.
What is the open time of your waterborne adhesive?
8–15 minutes for the hand-wrapping version of R-5670 and 5–10 minutes for the automated-line version.
What does "wide activation window" mean?
The temperature range in which the adhesive activates fully. The automated version of R-5670 activates anywhere from 110°C to 140°C, so normal oven drift doesn't change the bond.
How fast does R-5670 build strength?
About 25 N/25 mm one minute after lamination and about 60 N/25 mm after 7 days. Full crosslinking takes 24 h at 23°C.
Can I convert 1,000 hours of aging into years of service?
No. Accelerated aging compares materials under a fixed condition. Validate the finished part to your OEM's durability standard.
Can you change the open time for my line?
Yes. Open time, activation temperature, solids and tack can be tuned. Custom samples take 7 working days.
Check the Window Against Your Line
Tell us your process, cycle time and durability standard. We'll recommend the grade, send the test reports and run a flat-panel test on your materials.
An engineer replies within 1 working day.