RELANETRELANET

Case Study · EV Door Panels

Nissan N7, N6 and NX7: 2K Waterborne PU Adhesive on EV Interior Trim

Nissan's interior programs leave little room for error: odor and VOC are pass/fail, every material is tested to Nissan's own methods, and the line can't wait. RELANET R-5670 two-component waterborne PU is in series production on the Dongfeng Nissan N7 and N6, with zero complaints on the N7 since launch. On the NX7, Nissan specified waterborne adhesive for a line that had been using solvent, and we spent two years with the Tier 1 to make it work. This EV door panel waterborne PU adhesive case study covers the N7, N6 and NX7 programs.

Door panel wrapped with RELANET R-5670 for Nissan EV program

Results at a glance

  • 3

    Nissan programs: N7, N6 (series production), NX7 (SOP scheduled)

  • 2 g/L

    VOC content of R-5670 (SGS, GB 33372; limit 50 g/L)

  • 22 of 22

    Listed substances not detected (Nissan VES M00-12, SGS, SOP-stage samples)

  • 5–10 N → fixed

    NX7 early peel vs. 19 N target; root cause found in the skin

  • 0

    Customer complaints on N7 since series production

Project at a Glance

Project at a Glance
ItemDetail
OEMDongfeng Nissan
Vehicle programsN7 (LK1A), N6 (LK2A), NX7 (LK2C)
PartsInterior wrapping; NX7 door panel (PP substrate, mesh fabric, PVC skin)
AdhesiveRELANET R-5670 two-component waterborne PU + R-60C curing agent (100 : 5–8 by weight)
CustomerNissan's Tier 1 door-panel supplier
StandardsNissan NES M0160; Nissan VES test methods for odor and emissions
N7 / N6 statusSeries production; waterborne adhesive in production on N7 from November 2025
NX7 statusSOP scheduled, after about two years of joint development
Field recordZero complaints on N7 since series production
RelationshipDongfeng Nissan programs are one of RELANET's two largest sources of business

Vehicle names identify the programs in RELANET's records and do not imply endorsement of this website by Nissan.

The Challenge

Japanese OEM Standards, an EV Cabin and a Line That Can't Stop

Japanese OEM Standards, an EV Cabin and a Line That Can't Stop
RequirementWhy it mattered
EmissionsOdor and VOC are veto items at Nissan. Since August 2025, Nissan has also asked suppliers to survey 22 specified solvent substances.
Nissan's own test methodsEach Japanese OEM uses its own standard; data from another OEM doesn't carry over.
Initial tack on curved trimSkins must hold on curves and folds straight out of the press, or edges spring back and blister.
Solvent to waterborne (NX7)The existing process ran on solvent adhesive; switching adds PP pretreatment and drying, and every adhesive change needs re-approval.
Skin variationThe adhesive bonds to the backing of the skin; a different knit cut peel strength by 40% on the same adhesive and process.

Emission Data from SOP-Stage Samples

SGS tested R-5670 specimens from the N7 (LK1A) program, produced on 27 August 2025, at SOP stage, using Nissan's VES methods. R-5670 is in series production as a Nissan N7 interior adhesive; these are its SOP-stage results.

Emission Data from SOP-Stage Samples
TestMethodResultSGS job no.
Odor intensity / irritationNissan VES M00-08 [N], method 2; 90°C × 4 h2.3 / 0GZAT2509006029LW01
Formaldehyde, acetaldehyde, acrolein, benzene, toluene, ethylbenzene, xylene, styrene, TVOCNissan VES M00-03 [N]; 65°C × 2 hAll not detectedGZAT2509006029LW03
22 listed substances + TVOCNissan VES M00-12 [N]; 60°C × 4 hAll not detectedGZAT2509006029LW02
VOC contentGB 33372-2020, Annex D2 g/L (limit 50 g/L)GZAT2603001821PC01
SGS VES test results for RELANET R-5670

“Nissan N7 is the program that best represents our environmental performance and our work to Japanese OEM standards.”

— He Bowen, founder of RELANET

NX7: Solvent to Waterborne, Specified by the OEM

This part of the case study is a solvent to waterborne adhesive conversion on the NX7 door panel.

NX7: Solvent to Waterborne, Specified by the OEM
ItemDetail
Starting pointThe Tier 1 was wrapping the part with solvent adhesive. Nissan specified waterborne adhesive for the NX7.
How we came inNissan knew RELANET's waterborne adhesive was already running on its programs and recommended that the Tier 1 work with us.
What changed on the linePP pretreatment added, solvent flash-off replaced by oven drying and activation, secondary IR activation before lamination
DurationAbout two years of joint development
StatusSOP scheduled

The Peel-Strength Investigation

5–10 N Against a 19 N Requirement. The Adhesive Wasn't the Problem.

During NX7 (K2C) development, initial peel strength reached only 5–10 N, whatever was tried. Nissan required 19 N. The customer had never validated the skin on its own.

The Peel-Strength Investigation
StepWhat we didWhat we found
1Repeated the test with the same adhesive and processResults stayed at 5–10 N
2Cross-tested: bonded different skins with the same adhesive, and the same skin with different settingsThe low result followed the skin, not the adhesive or the settings
3Compared with another Nissan program on the same adhesive and processPVC with knit backing on the Teana: 12.7 N; on the K2C skin: 7.6 N, a 66.8% difference
4Traced the causeThe knit fabric chosen for the skin backing
5Fix (by the customer, close to SOP)An added nonwoven layer on the skin, which solved both the low peel strength and the blistering
Peel strength before and after skin fix, 5–10 N vs 19 N

NX7 (K2C) early peel vs. requirement

  • K2C skin, early trials5–10 N
  • Nissan requirement19 N

Same adhesive and process, different skin

  • Teana (PVC with knit backing)12.7 N
  • K2C skin7.6 N

66.8% difference

Why it matters for you: the adhesive bonds to the back of the skin. If the skin's backing isn't defined and tested, peel data isn't comparable, and the adhesive gets blamed for a material problem. We test the actual production skin before SOP.

The Door-Panel Process

NX7 (LK2C) door-panel wrapping · R-5670 + R-60C · PP substrate, mesh fabric, PVC skin

  1. 1

    Step 1

    Robotic spraying

  2. 2

    Step 2

    Drying and activation

  3. 3

    Step 3

    Secondary infrared activation

  4. 4

    Step 4

    Mesh-fabric lamination

  5. 5

    Step 5

    Pressing and forming

We record dimensions, coat weight, temperatures and cycle time at every trial and turn the validated parameters into the work instruction.

R-5670 performance on this type of construction (typical specimen results)

R-5670 performance on this type of construction (typical specimen results)
ItemValue
Peel at 1 minuteAbout 25 N/25 mm
Peel at 7 daysAbout 60 N/25 mm
Test combinationPVC with knitted backing on flame-treated PP
Activation window, automated version110–140°C
Humidity aging85% peel retention after 60°C / 95% RH × 1,000 h
Door-panel wrapping process with waterborne PU adhesive

Supply When the Line Speeds Up

On the Dongfeng Nissan Teana program in Xiangyang, the build schedule was planned at about 8,000 vehicles a month. Actual demand reached 13,000, so the plant added weekend shifts. The order came three days before the adhesive was needed, with delivery due in two days. We ran rush production and delivered, and the customer's line didn't stop.

R-5670 is held as standard stock, with annual capacity of about 960 tonnes across the product range.

Traceable on Every Program

  • National materials database. For these published vehicle programs, RELANET's materials are registered in China's national automotive materials database, which records every material used in a vehicle model and traces it back to the supplier.
  • Registered with the OEM. R-5670 was recorded in the OEM's program files early in development.
  • Batch traceability. About 250 ml retained from every batch; batch viscosity variation ≤3%.
  • Quality system. IATF 16949 (IATF/T19001-2026), ISO 9001, ISO 14001, ISO 45001.

What This Means for Your Program

  1. 1

    Test emissions to your OEM's own method, at SOP stage. Data from production samples, by the OEM's method, is what the materials engineer can sign off.

  2. 2

    Validate the skin before blaming the adhesive. Cross-test skins and settings; the backing decides the result.

  3. 3

    Plan a solvent-to-waterborne switch as a project, not a product swap. Pretreatment, drying and re-approval take time; NX7 took about two years.

  4. 4

    Choose a supplier that can ship when volumes jump. A three-day order shouldn't stop your line.

Other RELANET grades at Nissan: R-7110 APAO in series production on the Dongfeng Nissan Sylphy; R-7206 APAO approved by Nissan for series production.

FAQ

  • Which Nissan models use RELANET R-5670?

    The Dongfeng Nissan N7 (LK1A) and N6 (LK2A) in series production, and the NX7 (LK2C) with SOP scheduled.

  • Did R-5670 pass Nissan's emission tests?

    SGS tested SOP-stage N7 samples by Nissan VES methods: odor intensity 2.3 with zero irritation; aldehydes, aromatics, TVOC and all 22 listed substances not detected.

  • What caused the low peel strength on NX7?

    The knit fabric on the skin backing. Peel was 5–10 N against a 19 N target; an added nonwoven layer solved it.

  • How long did the solvent-to-waterborne conversion take?

    About two years of joint development with the Tier 1, from the OEM's waterborne specification to scheduled SOP.

  • Has R-5670 had complaints on N7?

    No. Zero customer complaints since series production.

Bringing Waterborne PU onto Your Door-Panel Line?

Send us your skin, substrate, process and OEM standard. We'll test the real materials, pre-test to the OEM's method and plan the trial with you.

An engineer replies within 1 working day.All case studies