Solutions · Solvent to Waterborne
Converting Interior Wrapping Lines from Solvent to Waterborne Adhesive
About 60% of interior lamination in South China still runs on solvent adhesive, most of it on long-running Japanese-brand programs. OEM VOC requirements, worker health and the cost of handling flammable chemicals are pushing those lines to change. RELANET has moved wrapping lines from solvent to waterborne adhesive on Nissan programs, and this page shows what changes on the line, what it costs, how long re-approval takes and where conversions usually go wrong. It is a practical guide to solvent to waterborne adhesive conversion for interior trim lines.

~60%
Share of South China interior lamination still on solvent (typical estimate)
500 g vs. 100 g
Solids per kg: waterborne vs. solvent adhesive
6 months
Typical time for one OEM re-test round after an adhesive change
2 g/L
VOC content of R-5670 (SGS, GB 33372; limit 50 g/L)
Why Plants Convert
Five Reasons Lines Leave Solvent Adhesive
1. OEM VOC and odor requirements. This is the most common trigger we see. OEMs pass emission targets down to their Tier 1s, and an adhesive full of solvent is the obvious thing to change. Since August 2025, Nissan has asked its interior suppliers to survey 22 specified solvent substances in their materials. R-5670 showed none of the 22 substances on Nissan's VES M00-12 list (SGS).
2. Government pressure. In 2023, Guangzhou authorities issued an official notice requiring plants to eliminate solvent-based adhesives. Workers stopped the lines and the authorities compromised. The requirement eased; the direction didn't. Plants that use a lot of solvent remain a focus for environmental inspections.
3. Worker health. On solvent lines, operators often wear masks and the workshop smells all year. Waterborne adhesive has no harsh solvent odor, and occupational-health checks become routine instead of a recurring problem.
4. The hazardous-chemical burden. Solvent adhesive is flammable. Every step of the chain, from manufacturing and transport to storage and use at the Tier 1, needs dangerous-chemicals qualification, fire protection and explosion-proof ventilation. Waterborne adhesive is not classified as a hazardous chemical, is non-flammable and non-explosive, and ships as non-dangerous goods with a sea-transport safety appraisal certificate.
5. Japanese programs are the largest remaining pool. About 70% of Japanese-brand vehicles built in China still use solvent adhesive in interior lamination (typical estimate). The process was fixed years ago and has never been revisited. The technology to replace it exists; the barrier is the process change. As new programs launch, OEMs such as Nissan now specify waterborne adhesive from the start.
What It Costs
Solvent vs. Waterborne: The Numbers
This waterborne vs. solvent-based adhesive comparison uses typical estimates from RELANET customer projects in China.
| Cost item | Solvent adhesive | Waterborne adhesive (RELANET) | Note |
|---|---|---|---|
| Active content per kg | About 100 g | About 500 g (R-5670: 47–50% solids) | Less material to buy, ship and store per m² |
| Coat weight per part | Baseline | 20–30% lower | Typical estimate; depends on part and spray setup |
| Unit price | Baseline | In China, often at or below solvent adhesive per kg | Solvent price includes dangerous-goods handling along the chain |
| Spray-line extraction (activated-carbon filtration + exhaust ducting) | Typically RMB 0.8–1 million (≈ USD 110,000–140,000) | Spray lines still need extraction; no explosion-proof design for the adhesive itself | Typical estimate for a solvent spray line |
| Hazardous waste disposal | RMB 100,000–200,000 per year (≈ USD 14,000–28,000) | RMB 100,000–200,000 per year | Wash water and residues from waterborne lines still go to licensed disposal |
| Explosion-proof ventilation and fire retrofit | Required | Not required for the adhesive | Waterborne is non-flammable |
| Dangerous-goods transport and storage | Required | Not required | Ships as non-dangerous goods |
| Added process steps | — | PP pretreatment + drying oven (see below) | The real cost of conversion |
Active content per kg
- Solvent adhesive
- About 100 g
- Waterborne adhesive (RELANET)
- About 500 g (R-5670: 47–50% solids)
- Note
- Less material to buy, ship and store per m²
Coat weight per part
- Solvent adhesive
- Baseline
- Waterborne adhesive (RELANET)
- 20–30% lower
- Note
- Typical estimate; depends on part and spray setup
Unit price
- Solvent adhesive
- Baseline
- Waterborne adhesive (RELANET)
- In China, often at or below solvent adhesive per kg
- Note
- Solvent price includes dangerous-goods handling along the chain
Spray-line extraction (activated-carbon filtration + exhaust ducting)
- Solvent adhesive
- Typically RMB 0.8–1 million (≈ USD 110,000–140,000)
- Waterborne adhesive (RELANET)
- Spray lines still need extraction; no explosion-proof design for the adhesive itself
- Note
- Typical estimate for a solvent spray line
Hazardous waste disposal
- Solvent adhesive
- RMB 100,000–200,000 per year (≈ USD 14,000–28,000)
- Waterborne adhesive (RELANET)
- RMB 100,000–200,000 per year
- Note
- Wash water and residues from waterborne lines still go to licensed disposal
Explosion-proof ventilation and fire retrofit
- Solvent adhesive
- Required
- Waterborne adhesive (RELANET)
- Not required for the adhesive
- Note
- Waterborne is non-flammable
Dangerous-goods transport and storage
- Solvent adhesive
- Required
- Waterborne adhesive (RELANET)
- Not required
- Note
- Ships as non-dangerous goods
Added process steps
- Solvent adhesive
- —
- Waterborne adhesive (RELANET)
- PP pretreatment + drying oven (see below)
- Note
- The real cost of conversion
Typical estimates from RELANET customer projects in China. Your figures depend on line size, local regulation and disposal contracts.
The honest summary: converting doesn't make hazardous waste go away, and you'll add pretreatment and drying. What you remove is the flammable-solvent burden: fire risk, explosion-proof equipment, dangerous-goods handling and solvent odor. You also use 20–30% less adhesive per part.
- Waterborne adhesive~500 g
- Solvent adhesive~100 g
What Changes on the Line
Four Steps Become Five
| Step | Solvent hand wrapping (today) | Waterborne PU hand wrapping |
|---|---|---|
| 1 | — | PP substrate pretreatment (flame or plasma)new |
| 2 | Spray substrate | Spray substrate |
| 3 | Spray skin | Spray skin |
| 4 | Flash off solvent | Drying ovenchanged |
| 5 | Hand wrapping | Hand wrapping |
1
- Solvent hand wrapping (today)
- —
- Waterborne PU hand wrapping
- PP substrate pretreatment (flame or plasma)new
2
- Solvent hand wrapping (today)
- Spray substrate
- Waterborne PU hand wrapping
- Spray substrate
3
- Solvent hand wrapping (today)
- Spray skin
- Waterborne PU hand wrapping
- Spray skin
4
- Solvent hand wrapping (today)
- Flash off solvent
- Waterborne PU hand wrapping
- Drying ovenchanged
5
- Solvent hand wrapping (today)
- Hand wrapping
- Waterborne PU hand wrapping
- Hand wrapping
Solvent adhesive doesn't need you to know much about the substrate; waterborne adhesive does. That's why pretreatment is the new step.
Solvent hand wrapping (today)
- 1Spray substrate
- 2Spray skin
- 3Flash off solvent
- 4Hand wrapping
Waterborne PU hand wrapping
- 1PP substrate pretreatment (flame or plasma) (New or changed step)
- 2Spray substrate
- 3Spray skin
- 4Drying oven (New or changed step)
- 5Hand wrapping
New or changed step
RELANET R-5670 hand-wrapping version, typical settings
| Parameter | Value |
|---|---|
| Mix ratio | R-5670 : R-60C = 100 : 5–8 (by weight) |
| Coat weight | 80–110 g/m² per side |
| Drying | 10–25 min at room temperature, or 3–8 min in an 80°C oven |
| Activation | 65–85°C |
| Open time | 8–15 min |
| Initial tack | About 25 N/25 mm at 1 minute |
| Full crosslinking | 24 h at 23°C |
| Gun cleaning | Water |
Mix ratio
- Value
- R-5670 : R-60C = 100 : 5–8 (by weight)
Coat weight
- Value
- 80–110 g/m² per side
Drying
- Value
- 10–25 min at room temperature, or 3–8 min in an 80°C oven
Activation
- Value
- 65–85°C
Open time
- Value
- 8–15 min
Initial tack
- Value
- About 25 N/25 mm at 1 minute
Full crosslinking
- Value
- 24 h at 23°C
Gun cleaning
- Value
- Water
For automated lines, the automated version activates anywhere from 110°C to 140°C.
Four Things Plants Miss When They Convert
- 1
A passing dyne reading isn't enough. After flame or plasma treatment, laminate within 4 hours. After that, active groups on the PP surface fade while the dyne value still looks fine. High temperatures shorten the window further.
- 2
Wrap from the deepest point outward. Start at the lowest point of a deep cavity and work out to the edge fold, so no air or stress is trapped.
- 3
Limit tenons and clips. Too many tenon positions get in the way of edge folding.
- 4
Keep hand-wrapped parts small. For manual wrapping, keep parts within 80 cm × 40 cm. Larger parts heat unevenly from front to back, and the adhesive activates unevenly.
The Trade-Offs, and How We Handle Them
What Gets Harder with Waterborne Adhesive
| Trade-off | Why it happens | What we do |
|---|---|---|
| PP needs pretreatment | Water-based adhesive can't wet untreated PP (surface energy ≈ 24 mN/m) | Flame or plasma, laminated within 4 h; where flame isn't allowed, PP primers R-132 / R-136 |
| Drying takes longer than flashing off solvent | Water evaporates more slowly than solvent | Staged oven drying (60°C → 80°C on automated lines; 80°C × 3–8 min for hand wrapping); grades tuned to your oven length |
| Flame and solvent can't share a floor | Flame treatment for waterborne lines next to solvent spray booths is a fire risk | Plan the changeover by area or by line; never run both in the same zone |
| Humid seasons | Slow drying and blushing (white film) after lamination | Solids, activation temperature and open time adjusted to your plant's climate, on site |
| Cold workshops | Adhesive film loses elongation | Hand-wrapping version keeps 600–1,000% elongation at 10°C |
| Frost in storage and transport | Waterborne adhesive must not freeze | Store and ship above 5°C; insulated transport for cold regions |
| Re-approval | A new adhesive must pass the OEM tests again | Pre-validation testing to the OEM standard before submission (see the plan below) |
PP needs pretreatment
- Why it happens
- Water-based adhesive can't wet untreated PP (surface energy ≈ 24 mN/m)
- What we do
- Flame or plasma, laminated within 4 h; where flame isn't allowed, PP primers R-132 / R-136
Drying takes longer than flashing off solvent
- Why it happens
- Water evaporates more slowly than solvent
- What we do
- Staged oven drying (60°C → 80°C on automated lines; 80°C × 3–8 min for hand wrapping); grades tuned to your oven length
Flame and solvent can't share a floor
- Why it happens
- Flame treatment for waterborne lines next to solvent spray booths is a fire risk
- What we do
- Plan the changeover by area or by line; never run both in the same zone
Humid seasons
- Why it happens
- Slow drying and blushing (white film) after lamination
- What we do
- Solids, activation temperature and open time adjusted to your plant's climate, on site
Cold workshops
- Why it happens
- Adhesive film loses elongation
- What we do
- Hand-wrapping version keeps 600–1,000% elongation at 10°C
Frost in storage and transport
- Why it happens
- Waterborne adhesive must not freeze
- What we do
- Store and ship above 5°C; insulated transport for cold regions
Re-approval
- Why it happens
- A new adhesive must pass the OEM tests again
- What we do
- Pre-validation testing to the OEM standard before submission (see the plan below)
Line Conversion Checklist
What to Prepare Before the First Trial
Line Conversion Checklist
- Drying oven: length, temperature zones and line speed. Can it hold 60–80°C?
- PP pretreatment: flame, plasma or primer; where the station sits; how you'll keep the 4-hour window.
- Fire separation: flame stations away from any remaining solvent booths.
- Spray equipment: guns and lines flushed of solvent; switched to water cleaning.
- Storage: adhesive and curing agent kept above 5°C, sealed, away from frost.
- Skins and substrates: 1–2 m² of each for flat-panel tests. Note the skin's backing (knit, nonwoven) — it can decide the result.
- Your OEM's material standard: the current spec and test list.
- Waste handling: a disposal contract for wash water and adhesive residues.
Get the full checklist (PDF) with oven, pretreatment and trial-record templates:
Conversion Plan and Timeline
Plan for Re-Approval Before You Change the Adhesive
| Item | Typical figure | Note |
|---|---|---|
| One OEM re-test round after an adhesive change | At least 6 months, RMB 20,000–30,000 (≈ USD 2,800–4,200) | Typical estimate |
| Certification testing for a new project | RMB 50,000–150,000 per project (≈ USD 7,000–21,000) | Typical estimate |
| Full OEM material approval | 6–18 months | Varies by OEM and part |
| From validation pass to series production | About 6 months | Typical |
| NX7 program, solvent → waterborne (joint development) | About 2 years to SOP | See case below |
One OEM re-test round after an adhesive change
- Typical figure
- At least 6 months, RMB 20,000–30,000 (≈ USD 2,800–4,200)
- Note
- Typical estimate
Certification testing for a new project
- Typical figure
- RMB 50,000–150,000 per project (≈ USD 7,000–21,000)
- Note
- Typical estimate
Full OEM material approval
- Typical figure
- 6–18 months
- Note
- Varies by OEM and part
From validation pass to series production
- Typical figure
- About 6 months
- Note
- Typical
NX7 program, solvent → waterborne (joint development)
- Typical figure
- About 2 years to SOP
- Note
- See case below
Typical estimates from RELANET projects in China.
Check your OEM spec before you start. Material standards at Japanese OEMs, including Nissan, Honda and Toyota, were written when interior lines used solvent adhesive. Some drying and test conditions reflect solvent behavior. When you convert, review those clauses with the OEM so the waterborne process is judged on the right conditions.
How we run a conversion (our eight-step project flow)
- 01
You share substrate, skin and process; we review them.
- 02
You send 1–2 m² of skin and substrate; we test flat panels.
- 03
We report feasibility and any material changes needed.
- 04
Both teams trial the system on real parts and equipment.
- 05
We record coat weight, temperatures, dimensions and cycle time.
- 06
We compile part-level data for your submission to the OEM.
- 07
We propose the process instruction, or revise and re-trial until it passes.
- 08
SOP, then supply and technical follow-up.
Case: Nissan NX7
The OEM Specified Waterborne. The Tier 1 Had Been Using Solvent.
- Program
- Nissan NX7 (LK2C) door-panel wrapping
- Starting point
- Solvent adhesive on the existing process; Nissan specified waterborne adhesive for the program
- System
- R-5670 + R-60C on PP, with mesh fabric and PVC skin; robotic spraying, drying and activation, secondary IR activation, lamination, pressing
- Problem found
- Early peel strength was only 5–10 N against a 19 N target. Cross-testing traced it to the knit backing of the skin, not the adhesive.
- Duration
- About 2 years of joint development
- Status
- SOP scheduled
Vehicle names identify programs in RELANET's records and do not imply endorsement of this website by Nissan.
Which Waterborne Adhesive Replaces What
Match the Replacement to the Solvent Adhesive You Use Now
To replace solvent-based adhesive in an automotive interior, match the waterborne grade to the solvent adhesive and parts you have today; for a solvent-free adhesive for car interior lines without a drying oven, see the two routes below the table.
| You use today | Typical parts | Replace with | Why |
|---|---|---|---|
| Solvent chloroprene contact cement ("yellow glue") on porous materials | Foam, felt, acoustic insulation, nonwovens | R-5110 waterborne chloroprene | Fast tack on porous materials; press 1–10 s at 20°C; in production on FAW Toyota Corolla acoustic parts |
| Solvent chloroprene or solvent PU on wrapped trim | Door panels, instrument panels, armrests, seats | R-5670 2K waterborne PU | ~25 N/25 mm at 1 min; 2 g/L VOC; series supply on Nissan N7 / N6 |
| Solvent adhesive on backlit trim | Light-transmitting skins | R-5610 optical waterborne PUD | Waterborne and light-transmitting; in production on GAC Toyota V57 |
Solvent chloroprene contact cement ("yellow glue") on porous materials
- Typical parts
- Foam, felt, acoustic insulation, nonwovens
- Replace with
- R-5110 waterborne chloroprene
- Why
- Fast tack on porous materials; press 1–10 s at 20°C; in production on FAW Toyota Corolla acoustic parts
Solvent chloroprene or solvent PU on wrapped trim
- Typical parts
- Door panels, instrument panels, armrests, seats
- Replace with
- R-5670 2K waterborne PU
- Why
- ~25 N/25 mm at 1 min; 2 g/L VOC; series supply on Nissan N7 / N6
Solvent adhesive on backlit trim
- Typical parts
- Light-transmitting skins
- Replace with
- R-5610 optical waterborne PUD
- Why
- Waterborne and light-transmitting; in production on GAC Toyota V57
Don't want a drying oven at all?
Two solvent-free routes skip drying entirely:
Frequently Asked Questions
Is waterborne adhesive as strong as solvent adhesive?
On wrapped interior parts, yes. In BYD interior testing, R-5670 broke the substrate in every specimen, at room temperature, after 90°C × 168 h and after 10 damp-heat cycles. Peel strength on PVC with knitted backing reaches about 60 N/25 mm after 7 days.
What changes on the line?
Two steps: PP pretreatment (flame, plasma or primer) and an oven drying step in place of solvent flash-off. Spray guns are cleaned with water.
Does waterborne adhesive eliminate hazardous waste?
No. Wash water and residues still need licensed disposal, typically RMB 100,000–200,000 per year for a Tier 1 plant, for either system. What disappears is the flammable-solvent burden: fire risk, explosion-proof ventilation and dangerous-goods handling.
How long does re-approval take?
Plan for at least 6 months and RMB 20,000–30,000 per OEM re-test round (typical estimate). Full material approval at an OEM usually takes 6–18 months.
Can I run solvent and waterborne lines in the same workshop?
Not in the same zone. Flame treatment for PP next to solvent spraying is a fire risk. Convert by area or by line.
Does waterborne adhesive cost more?
In China, waterborne adhesive is often priced at or below solvent adhesive per kg, and parts use 20–30% less adhesive by weight (typical estimate). The added cost is pretreatment and drying.
Which RELANET adhesive replaces solvent contact cement?
R-5110 for foam, felt and acoustic parts; R-5670 for wrapped door panels, instrument panels, armrests and seats.
Request a Conversion Assessment
Send us your part, current solvent adhesive, skin, substrate and line setup. We'll recommend the waterborne grade, list the line changes and plan the OEM re-test with you.
Start your solvent to waterborne adhesive conversion with a free assessment.
An engineer replies within 1 working day.