Material Compatibility

Material-Pair Compatibility: Skin × Substrate × Adhesive

An interior bond is never just "adhesive on plastic". It is a skin, an adhesive and a substrate, and the weakest link decides the result. Use this chart to find the RELANET adhesive for your TPO, PVC, leather, fabric and PP combinations, see which pairs are already proven, and send us your own materials for a free test.

Looking for an adhesive for TPO, PVC, leather and PP substrates? Start with the chart below.

Flat lay of interior skin and substrate samples: PVC, TPO, leather, microfiber, 3D mesh, flocked fabric, PP, ABS and honeycomb

The Problem

"It bonded fine on the sample. On our skin, it didn't."

Most bonding surprises come from the material pair, not the adhesive:

  • The skin changes, and the result changes. A new PVC lot or a different knit backing can drop peel strength sharply.

  • Low-surface-energy plastics. PP and IXPP need treatment before most adhesives will wet them.

  • Hidden chemistry. Plasticizers migrate out of soft PVC; release agents stay on molded parts; regrind changes the surface.

  • Heat-sensitive skins. Thin leather and ultra-soft skins shrink or mark at high activation temperatures.

  • Porous materials. Foam, felt and honeycomb soak up adhesive and starve the bond line.

Compatibility Chart

Key:

  • Production-proven (series production or OEM test)
  • Lab data available
  • Recommended starting grade, to be tested on your materials
  • "Ask us" = send us the pair and we'll recommend a grade
  • PVC with knitted backing

    Flame-treated PP:
    Production-proven (series production or OEM test): R-5670
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-5670, R-5610
    Wood-plastic / natural-fiber board:
    Lab data available: R-5670(≥1,050 N/m)

    Other substrates: ask us

  • PU leather

    Flame-treated PP:
    Recommended starting grade, to be tested on your materials: R-5670
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-5670, R-5610

    Other substrates: ask us

  • TPO

    Flame-treated PP:
    Lab data available: R-5670(≥980 N/m on modified PP)
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-5610

    Other substrates: ask us

  • Genuine leather

    Flame-treated PP:
    Recommended starting grade, to be tested on your materials: R-9610
    Clean PP (untreated):
    Recommended starting grade, to be tested on your materials: R-9610
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-9610
    Foam (EVA / PU):
    Lab data available: R-5670(≥1,300 N/m on EVA)

    Other substrates: ask us

  • Microfiber

    Flame-treated PP:
    Recommended starting grade, to be tested on your materials: R-9610
    Clean PP (untreated):
    Recommended starting grade, to be tested on your materials: R-9610
    ABS / PC-ABS:
    Lab data available: R-5670(≥1,150 N/m)

    Other substrates: ask us

  • Suede

    Flame-treated PP:
    Recommended starting grade, to be tested on your materials: R-9610
    Clean PP (untreated):
    Recommended starting grade, to be tested on your materials: R-9610
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-5610, R-9610

    Other substrates: ask us

  • 3D mesh fabric

    Flame-treated PP:
    Production-proven (series production or OEM test): R-5670
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-5610

    Other substrates: ask us

  • Flocked / knitted fabric

    Flame-treated PP:
    Production-proven (series production or OEM test): R-5670
    Clean PP (untreated):
    Production-proven (series production or OEM test): R-7110
    ABS / PC-ABS:
    Recommended starting grade, to be tested on your materials: R-7110
    PHC paper honeycomb:
    Production-proven (series production or OEM test): R-5670
    Foam (EVA / PU):
    Recommended starting grade, to be tested on your materials: R-5110

    Other substrates: ask us

  • Foam, felt, nonwoven

    Flame-treated PP:
    Recommended starting grade, to be tested on your materials: R-7110
    Clean PP (untreated):
    Recommended starting grade, to be tested on your materials: R-7110
    Foam (EVA / PU):
    Production-proven (series production or OEM test): R-5110

    Other substrates: ask us

  • Light-transmitting skins and films

    Flame-treated PP:
    Production-proven (series production or OEM test): RY-10
    Clean PP (untreated):
    Production-proven (series production or OEM test): RY-10(no surface treatment)
    ABS / PC-ABS:
    Production-proven (series production or OEM test): RY-10Recommended starting grade, to be tested on your materials: R-5610
    PC / PMMA (optical):
    Lab data available: R-60(>40 N/25 mm)

    Other substrates: ask us

Proof behind ● entries: PVC with knitted backing and 3D mesh on flame-treated PP (Nissan door-panel programs, R-5670); flocked fabric on flame-treated PP and sand-blasted PHC honeycomb (BYD interior test, substrate failure, R-5670); fabric on PP (R-7110, batch production on seat covers, door trim strips and headliners); foam and felt (R-5110, FAW Toyota Corolla acoustic parts); light-transmitting film on PP, ABS and PC (RY-10, Honda Ye P7 / Ye S7). ◐ values are typical lab results, 180° peel, 24 h after cure.

Your pair isn't proven here yet? That's what our flat-panel test is for.

Substrates and Skins in Detail

PP and IXPP

Need an adhesive for PP without primer? APAO hot melts and RY-10 film bond PP directly.

Why it's hard: PP and IXPP have a surface energy of about 24 mN/m, far below the ≥38 mN/m needed for cohesive failure. Release agents, regrind and contamination make it worse.

Your options:

  • Bond without pretreatment: R-7110 and R-7206 APAO hot melts bond PP and ABS directly, without sanding or primer.
  • Waterborne PU after treatment: flame, corona or plasma treat the PP, then wrap within 4 hours. R-5670 is proven on flame-treated PP.
  • Light-transmitting parts: RY-10 bonds PP directly without surface treatment. For R-5610, flame-treat PP and back-coat IXPP.

ABS, PC/ABS and PC

Surface energy around 28–32 mN/m, easier than PP but still below the target for many skins. R-7110 and R-7206 bond ABS directly; R-5610 and RY-10 bond ABS and PC; microfiber on ABS reaches ≥1,150 N/m with waterborne PU.

TPO Skins

TPO skin adhesive options: R-5670 for wrapping TPO on modified PP, R-5610 for backlit TPO.

Common on instrument panels, including IMG and vacuum-formed parts. TPO on modified PP reaches ≥980 N/m with waterborne PU in lab testing. For backlit TPO skins, use R-5610.

PVC and PU Leather

The adhesive usually bonds to the knit backing, not the PVC itself, so the knit decides much of the peel (see Section 6). Soft PVC releases plasticizer over time; RELANET waterborne PU resists silicone-oil and plasticizer migration, so PVC skins don't soften and lift. PVC on wood-plastic board reaches ≥1,050 N/m.

Genuine Leather, Microfiber and Suede

As a leather wrapping adhesive for automotive interiors, use R-5670 waterborne PU or R-9610 PUR.

High-end skins on armrests, consoles and instrument panels. Genuine leather on EVA foam reaches ≥1,300 N/m with waterborne PU; microfiber on ABS ≥1,150 N/m. R-9610 PUR is designed for PP and ABS with genuine leather, microfiber or suede, with ≥500% elongation for 3D wraps. Thin leather shrinks when overheated: the hand-wrapping version of R-5670 activates at 65–85°C, and R-9692 PUR offers low-temperature activation.

Fabrics, 3D Mesh and Flocked Fabric

3D mesh on flame-treated PP runs in Nissan door-panel production with R-5670 (robotic spray, IR activation, mesh lamination). Flocked fabric on PP and paper honeycomb passed BYD interior testing with substrate failure. R-7110 bonds fabrics and foam to PP for edge folding and seat covers.

Foam, Felt and Nonwovens

Porous materials soak up adhesive. R-5110 waterborne chloroprene penetrates quickly, builds tack on contact and presses in 1–10 s at 20°C. Confirm foam density, porosity and coat weight before production.

Paper Honeycomb (PHC) Boards

Lightweight load floors and spare wheel covers. Sand-blast the board, spray 80 g/m² per side, dry 80°C × 5 min, press 0.2 MPa × 15 s and cure 7 days. In BYD interior testing, flocked fabric on PHC held 28.8 N at room temperature, 30.7 N after 90°C × 168 h and 29.5 N after 10 humidity cycles, all with substrate failure.

Optical PC, PMMA and Glass

For light guides, transparent panels and smart surfaces. R-60 optical-grade film reaches >40 N/25 mm on optical PC, PMMA and glass, with >99% transmittance (new product). RY-10 bonds PC directly.

PP Primers: R-132 and R-136

When your process requires pretreatment, RELANET PP primers improve adhesion on polypropylene before lamination.

  • Type

    R-132 PP primer
    Solvent-based chlorinated polyolefin primer
    R-136 silane-modified PP primer
    Silane-modified primer
  • Application

    R-132 PP primer
    Brush, wipe or spray, thin even coat
    R-136 silane-modified PP primer
    Brush, wipe or spray
  • Flash-off

    R-132 PP primer
    5–10 min at room temperature
    R-136 silane-modified PP primer
    5–10 min at room temperature
  • Bond within

    R-132 PP primer
    30 min to 4 h after application
    R-136 silane-modified PP primer
    30 min to 4 h after application
  • Packaging

    R-132 PP primer
    1 kg / 5 kg
    R-136 silane-modified PP primer
    1 kg / 5 kg

Primer for interior trim lamination: use it where flame or plasma treatment isn't available, or near solvent stations where an open flame is not allowed.

Flame treatment of a plastic surface, the alternative to a PP primer

Why the Skin Matters

Same Adhesive, Same Process, 66.8% Different Peel

Two PVC skins with knitted backing were bonded with the same adhesive and the same process. Average peel was 12.7 N on one and 7.6 N on the other, a 66.8% difference. The adhesive bonds to the knit fabric on the back of the PVC, so the knit's material and structure caused the difference, not the adhesive.

On another program, early peel was only 5–10 N against a 19 N target. Cross-testing traced it to the skin's knit fabric, and adding a nonwoven layer met the target.

What this means for you: fix the skin specification before adhesive approval, and test the exact skin lot you will use in production.

Average peel, same adhesive and process
  • PVC skin with knitted backing A12.7 N
  • PVC skin with knitted backing B7.6 N
Where the adhesive bonds
  1. PVC skin
  2. Knitted backing: the adhesive bonds here
  3. Adhesive
  4. Substrate

Material Watch-Outs

  • Expired PP treatment

    What happens
    Active groups fade after about 4 hours; dyne reading still looks fine
    What to do
    Wrap within 4 hours; control the time, not just the dyne level
  • Release-agent residue

    What happens
    Adhesive bonds to the release agent; the whole skin peels after aging
    What to do
    Control mold release; clean parts
  • Regrind ratio changes

    What happens
    Surface properties shift batch to batch
    What to do
    Keep the regrind ratio stable; retest when it changes
  • Plasticizer migration (soft PVC)

    What happens
    Bond softens and lifts over time
    What to do
    Use a plasticizer-resistant adhesive; test after heat aging
  • Thin or ultra-soft skins

    What happens
    Shrink or mark at high activation temperatures
    What to do
    Lower activation (65–85°C hand-wrapping version, R-9692)
  • Porous foam and felt

    What happens
    Starved bond line
    What to do
    Adjust coat weight to porosity; use R-5110

Free Flat-Panel Test

Send Us 1–2 m² of Your Skin and Substrate

  1. 01

    You send 1–2 m² of skin and substrate.

  2. 02

    We test the material pair on flat panels, isolating materials and environment from process effects.

  3. 03

    You receive a report on feasibility and target compliance before any tooling or process change.

  4. 04

    If it passes, we move to a trial on your real parts.

This first step costs you nothing.

Frequently Asked Questions

  • Can your adhesive bond PP without primer?

    Yes. R-7110 and R-7206 APAO hot melts bond PP and ABS directly, without sanding or primer. RY-10 film also bonds PP directly. Waterborne PU needs flame, corona or plasma treatment on PP.

  • What's the best adhesive for TPO skins?

    For wrapping TPO on modified PP, R-5670 2K waterborne PU (≥980 N/m in lab tests). For backlit TPO, R-5610.

  • What do you recommend for leather wrapping?

    R-5670 for leather on foam (≥1,300 N/m on EVA), and R-9610 PUR for leather, microfiber and suede on PP or ABS.

  • Why did my peel drop when we changed the PVC supplier?

    The adhesive bonds to the knit backing. A different knit can change peel by more than half. Send us both skins and we'll compare.

  • My combination isn't in the chart. What now?

    Send us the pair. We'll recommend a starting grade and run a free flat-panel test.

Check Your Material Pair Before You Commit

Tell us your skin, substrate and process. We'll recommend a grade and test it on your materials.