RELANETRELANET

Case Study · Trunk and Spare Wheel Covers

BYD Denza Z9GT: Spare Wheel Cover Adhesive for Flocked Fabric on PP and Honeycomb

A spare wheel cover looks simple: a flat panel with fabric on top. But the flocked fabric has to stay bonded to flame-treated PP and paper honeycomb through summer heat, winter cold and damp, and the first adhesive on this BYD program didn't meet the standard. RELANET R-5670 did. It runs in series production on the BYD Denza Z9GT spare wheel cover, and in BYD HTE's formal interior test, every specimen broke in the material, not the bond.

Spare wheel cover laminated with flocked fabric using RELANET R-5670

Results at a glance

  • 9 / 9

    Specimens with substrate failure across three tests

  • 30.7 N

    Average peel after 90°C × 168 h (up from 28.8 N at room temperature)

  • 29.5 N

    Average peel after 10 damp-heat cycles, −40°C to 80°C

  • 2

    BYD programs with R-5670 in series production (Z9GT spare wheel cover, trunk lid trim)

  • Approved

    On BYD HTE's interior adhesive supplier list

Project at a Glance

Project at a Glance
ItemDetail
OEMBYD (HTE, Denza)
Vehicle programDenza Z9GT
PartTrunk spare wheel cover, laminated with flocked fabric
Tier 1 supplierGuangdong Yibin Auto Parts Co., Ltd.
AdhesiveRELANET R-5670 two-component waterborne PU + R-60C curing agent
SubstratesFlame-treated PP (front section of the cover); sand-blasted PHC paper honeycomb board
SkinFlocked fabric
StandardBYD interior standard
Formal test reportRJTSC-26-7-2-001 (tested 21 June – 1 July 2026, issued 2 July 2026)
StatusZ9GT spare wheel cover in series production; R-5670 also in series production on BYD trunk lid trim since May 2026
Supplier statusRELANET passed BYD HTE's interior adhesive audit and is on its approved supplier list

Vehicle names identify the programs in RELANET's records and do not imply endorsement of this website by BYD.

The Starting Point

The Previous Adhesive Didn't Meet the Standard

The program first ran with another supplier's adhesive, and it didn't meet BYD's interior standard. The part combines two very different substrates under one fabric:

The Previous Adhesive Didn't Meet the Standard
ChallengeWhy it's hard
Two substrates, one skinFlame-treated PP at the front of the cover and paper honeycomb (PHC) for the main board, both under the same flocked fabric
Porous honeycombPHC board absorbs adhesive; without the right surface preparation and coat weight, the bond line is starved
Large flat areaCoat weight and pressing pressure vary across a wide panel, leaving hollow spots
Trunk climateThe cover sees summer heat, winter cold and condensation; BYD tests at 90°C for a week and through −40°C / 80°C damp-heat cycles
Fast program paceBYD programs move quickly, with short notice on volumes

Switching to R-5670 brought the part to standard.

Construction and Process

The flocked fabric PP honeycomb lamination uses one adhesive system, R-5670 + R-60C, on both substrates.

Part build-up (top to bottom)

Part build-up (top to bottom)
AreaLayer 1Layer 2Layer 3
Front section of the coverFlocked fabricSprayed R-5670 + R-60CPP, flame-treated
Main boardFlocked fabricSprayed R-5670 + R-60CPHC paper honeycomb, sand-blasted
Flocked fabric on PP and PHC honeycomb layer structure

Front section of the cover

  1. 1Flocked fabric
  2. 2Sprayed R-5670 + R-60C
  3. 3PP, flame-treated

Main board

  1. 1Flocked fabric
  2. 2Sprayed R-5670 + R-60C
  3. 3PHC paper honeycomb, sand-blasted

Specimen preparation (as in the formal report)

Specimen preparation (as in the formal report)
StepSubstrate sideSkin side
Surface preparationPP: flame treatment · PHC: sand blastingFlocked fabric as supplied
Spray80 g/m² (one side)80 g/m² (one side)
Dry80°C × 5 min in oven80°C × 5 min in oven
Laminate0.2 MPa × 15 s
Cure7 days at 23 ± 5°C

Specimens made on 8 June 2026.

Test Results

All three tests were run to the BYD interior adhesive standard, and all three passed.

Test conditions

Test conditions
TestCondition
Room-temperature peel23 ± 3°C, 55% RH
Heat aging90 ± 2°C × 168 h, then 1 h at room temperature before testing
Cyclic damp heat(80°C × 15.5 h → RT 0.5 h → −40°C × 7.5 h → RT 0.5 h) × 10 cycles, then 1 h at room temperature

Results: PHC honeycomb + flocked fabric

Tested 29 June 2026; peel in N, as reported.

Results: PHC honeycomb + flocked fabric
TestSpecimen 1Specimen 2Specimen 3AverageFailure modeJudgment
Room temperature38.1522.4425.8128.80Substrate failure ×3Pass
Heat aging 90°C × 168 h26.6441.8723.4430.65Substrate failure ×3Pass
Cyclic damp heat × 1034.5428.3025.5729.46Substrate failure ×3Pass

What the numbers say

  • Every specimen failed in the material. The flocked fabric or honeycomb tore before the adhesive let go, so the bond is stronger than the materials around it.
  • No loss after aging. Average peel was 28.8 N at room temperature, 30.7 N after a week at 90°C and 29.5 N after ten damp-heat cycles.

Report conclusion (translated):

“Tested to BYD interior standards, RELANET two-component waterborne polyurethane R-5670 mixed with R-60C curing agent meets the requirements for bonding flocked fabric to PP board and PHC, and can be used for spare-wheel-cover lamination. Considering the interior styling, final confirmation should be based on testing of the actual product.”

— Formal test report RJTSC-26-7-2-001

The results table in the report shows the PHC group; the report's conclusion covers both the PP and the PHC constructions.

Peel strength after heat and humidity aging, BYD interior test

Average peel, N

  • Room temperature28.8 N

    substrate failure

  • Heat aging 90°C × 168 h30.7 N

    substrate failure

  • Cyclic damp heat × 1029.5 N

    substrate failure

Result page of the formal test report RJTSC-26-7-2-001
Result page of the formal test report RJTSC-26-7-2-001
Substrate failure on flocked fabric after humidity cycling
Substrate failure on flocked fabric after humidity cycling

Where the Test Was Done

The formal test was run in RELANET's laboratory in Huangpu, Guangzhou (Room 507, Building A1, Zhongju Science & Innovation City). Equipment used:

Where the Test Was Done
EquipmentModelCalibration valid untilAsset no.
Computerized tensile testerKJ-1065A15 Sep 2027QC-098
OvenKJ-1034A15 Sep 2027QC-056
Temperature-humidity chamberGuangkai HA40515 Jan 2027QC-78
Digital rotational viscometerSNB-2-J15 Sep 2027QC-091
Analytical balanceJA3003N15 Sep 2027QC-058
Hot peel testerZhonghao DZ-110-1KN10 Nov 2026QC-103

The Second BYD Program: Trunk Lid Trim

In May 2026, BYD approved R-5670 for trunk lid trim, and it went into series production. What mattered on that program: high initial tack (about 25 N/25 mm one minute after lamination), low VOC (2 g/L, SGS, GB 33372) and a stable cycle time.

Next on BYD spare wheel covers: R-9610 reactive PUR for a BYD spare-wheel-cover program, planned for series production.

Keeping Up with a Fast Program

BYD programs move fast, often without long forecasts or advance notice. R-5670 is a standard-stock grade, so orders ship from stock rather than waiting for a production run. Annual capacity across the range is about 960 tonnes.

What This Means for Your Trunk-Trim Part

  1. 1

    Prepare each substrate for what it is. Flame-treat PP; sand-blast honeycomb. One preparation doesn't fit both.

  2. 2

    Set coat weight on both sides. 80 g/m² on substrate and skin, dried before lamination, gave full substrate failure here.

  3. 3

    Test aging, not just room temperature. The bond should hold its strength after heat and damp-heat cycles, as it did here.

  4. 4

    Read the failure mode. Substrate failure means the adhesive is not the weak link; a clean adhesive failure points to preparation or process.

  5. 5

    Confirm on the real part. Flat specimens prove the material system; the actual part shape still needs testing.

Products Used

Products Used
ProductRole
R-5670 2K waterborne PUBonds flocked fabric to PP and PHC honeycomb on the Z9GT spare wheel cover; trunk lid trim
R-60C curing agentMixed with R-5670, 100 : 5–8 by weight
R-9610 reactive PURBYD spare-wheel-cover program planned

FAQ

  • Which adhesive is used on the BYD Denza Z9GT spare wheel cover?

    RELANET R-5670 two-component waterborne PU with R-60C curing agent, in series production.

  • Did R-5670 pass BYD's interior standard?

    Yes. In formal test report RJTSC-26-7-2-001, all three tests (room temperature, 90°C × 168 h, 10 damp-heat cycles) passed, with substrate failure on all nine specimens.

  • How do you bond flocked fabric to paper honeycomb?

    Sand-blast the PHC board, spray 80 g/m² on both the board and the fabric, dry at 80°C for 5 minutes, laminate at 0.2 MPa for 15 s and cure for 7 days.

  • Is RELANET an approved BYD supplier?

    RELANET passed BYD HTE's interior adhesive audit and is on its approved supplier list. R-5670 is also in series production on BYD trunk lid trim.

Laminating Fabric onto PP or Honeycomb?

Send us your fabric, substrate and the OEM standard. We'll prepare specimens the same way and send you the test report.

An engineer replies within 1 working day.All case studies